CDHumiston
Well-Known Member
I just heat treated two Alabama Damascus blades. I ramped my oven to 1550 and soaked the blades for 5 minutes. I quenched in AAA oil heated to 120. I finished the cooling in aluminum plates to avoid any warps. I tempered the blades at 350 for one hour and let the oven and blades cool to room temp.
I cleaned the blades and made sure there was no scale build up. My HRC reading on both blades was right at 51. Not good for me.
I decided to heat treat them again. Second time same procedure, but I cleaned them right after the aluminum plate cool down. Both are at 59 HRC.
I did a drop test on the blades to see if they are fragile and they had no issues with multiple drops at 5' on to a concrete floor.
Now the question...should I temper the blades again???
I cleaned the blades and made sure there was no scale build up. My HRC reading on both blades was right at 51. Not good for me.
I decided to heat treat them again. Second time same procedure, but I cleaned them right after the aluminum plate cool down. Both are at 59 HRC.
I did a drop test on the blades to see if they are fragile and they had no issues with multiple drops at 5' on to a concrete floor.
Now the question...should I temper the blades again???