8670 From Pop's

Randy Lucius

Well-Known Member
Anybody using 8670 from Pop's Knife Supply? I belong to Pop's Knife Supply Facebook group and people really seem to like it. Just wondering if anyone here has tried it. Thanks!
 
Austenitize: Heat to 1,560°-1,635° and hold for 5 minutes. Quench in oil.

Temper: Temper twice for two hours each time. Use the chart below to select the tempering temperature.
8670-TC.gif

From Alphaknife
From Pops

8670​

Hardening

Austenizing temperature - 1,550
Hold/Soak Time - 3-10 minutes
Expected Rc (as quenched) - 63-65

Oil Quench - Parks 50

Tempering

Temper twice for 2hrs.

300°F - 325°F - 62-63
375°F - 400°F - 61-62
Big difference in temper numbers.
 
Austenitize: Heat to 1,560°-1,635° and hold for 5 minutes. Quench in oil.

Temper: Temper twice for two hours each time. Use the chart below to select the tempering temperature.
8670-TC.gif

From Alphaknife
From Pops

8670​

Hardening

Austenizing temperature - 1,550
Hold/Soak Time - 3-10 minutes
Expected Rc (as quenched) - 63-65

Oil Quench - Parks 50

Tempering

Temper twice for 2hrs.

300°F - 325°F - 62-63
375°F - 400°F - 61-62
Big difference in temper numbers.
Thank you sir! Have you used this steel?
 
Back